JSR AT series for Tire applications
Transcription
JSR AT series for Tire applications
JSR Confidential JSR AT series for Tire applications JSR Corporation Petrochemical Products Div. Thermoplastic Elastomer Dept. This information contained herein is given in good faith but without any guarantee or warranty and involve proprietary rights of third parties. Our advice given in this information does not release you from the obligation to check its validity and to test our products as to their suitability for the intended process and uses. The application, use and processing of our products manufactured by you on the basis of our technical advice are beyond our control and, therefore, entirely on your own responsibility. Our products are sold only in accordance with Product Specification separately issued by us. 1 JSR Confidential JSR AT (Syndiotactic 1,2-Polybutadiene) JSR AT is Syndiotactic 1,2 Polybutadiene (JSR AT) for Tire applications. Melting point exists due to crystalline nature of Syndiotactic structure . JSR AT is the rubber with high hardness & low viscosity. Grade AT300 AT400 Form Pellet Pellet Packing 25kgs Bag 25kgs Bag Structure 1,2-Butadiene microstructure (%) 93 94 Crystallinity (%) 29 36 (mg/m3) 0.909 0.914 (℃) 105 126 (g/10min) 3.0 9.0 ML1+4 (120゚C) 15.3 - ML1+4 (130゚C) - 24.2 (Duro A) 91 94 M100 (MPa) 6.7 9.9 M300 (MPa) 13.5 17.1 Strength at break (MPa) 15.3 21.2 (%) 320 330 Non-Cure Properties Density Melting point MFR (150℃、21.2N) Cure Properties* Hardness Elongation at break *:Recipe;Polymer/ZnO/Stearic acid/Acc.DM**/Acc.TET**/S=100/3/2/1.5/0.66/1.6phr *Acc.DM ; Dibenzothiazyldisulfide *Acc.TET ; Tetra ethylthiuramdisulfide 2 JSR Confidential JSR AT series for Tire applications Tread Base tread (Belt) Bead Carcass Side wall S-SBR/BR NR/E-SBR NR/Phenol NR BR/NR Low Viscosity ◎ ◎ ◎ ◎ ◎ Decrease of consumption energy ◎ ◎ - ◎ ◎ High green strength ◎ ◎ ◎ ◎ ◎ Small mill shrinkage of sheet - ◎ - ◎ ◎ High-Hardness ◎ ◎ ◎ ◎ ◎ High-elastic shear modulus (G’) ◎ ◎ - ◎ ◎ - ◎ - ◎ - - ◎ - ◎ - Better Modulus(M300) ◎ ◎ ◎ - ◎ Better Tensile strength - - ◎ - - Better Tear strength - ◎ ◎ - ◎ Better crack growth - ◎ - ◎ ◎ Better Heat Resistance - ◎ ◎ ◎ - Component Base polymer Processability Driving stability Rolling Resistance Low 50℃ tanδ (by using Soft Carbon Black) Better Rolling Resistance (by decreasing content of Carbon Black) Physical properties Durability JSR AT is suitable for various tire applications. 3 JSR Confidential Effect of JSR AT for NR compound Recipe ; Run No. Ref-1 1 2 100 80 80 AT300 - 20 - AT400 - - 20 N330(HAF) 50 50 50 OIL(T-DAE) 10 10 10 NR(RSS#3) Stearic acid/ZnO/6C*1/CZ*2/S = 2.0/5.0/1.0/1.0/4.0 *1;N-(1,3-Dimethyl-butyl)-N’-phenyl-p-phenylendiamine *2;N-Cyclohexyl-2-benzothiazyl-sulfenamide(CBS) Mixing Procedure ; Mixer ; 250cc Laboratory-plastomill Stage 1 Tim (min) Ingredients Circulating Oil Temp. Rotor Speed 0.0 0.5 Polymer (NR) AT300orAT400,CB ZnO, Stearic Acid, 6C, Oil Clean up Damp at about 130oC 100oC 60rpm Batch from Stage 1 Accelerator, Sulfur Damp at about 100oC 70oC 60rpm 2.5 3.5 Stage 2 0.0 1.5 4 JSR Confidential Physical properties of unvulcanized rubber I. Viscosity & Properties of flow II. Extrusion test III.Green strength & Shrinkage ratio 5 I. Viscosity & Properties of flow Comp'd ML1+4 (125℃) Flow rate 【Flow rate test conditions】 1)Set temp;130℃ 2)Die size;2mm×2mmφ 3)Load;60kgf Excellent Excellent JSR Confidential Addition of AT decreases compound viscosity and increases flow rate. 6 JSR Confidential II. Extrusion test 〔Extruder Conditions〕 1)Cylinder & Die temp ; 100℃ 2)Die type ; Garvey die 3)Screw rotation ; 20rpm Ref-1 NR only 1 AT300 2 AT400 182% 155% 149% Edge Poor Good Excellent Surface Poor Good Excellent Run No. Die swell Sample Addition of AT improves extrudability. Especially, compound with At400 shows excellent extrudability. 7 JSR Confidential III. Green strength & Shrinkage ratio Green strength Excellent Excellent Shrinkage ratio 【Shrinkage test conditions】 1)Roll temp;60℃ 2)times;1minute 3)Measurement time;2 hours after Addition of AT increases green strength and decreases mill shrinkage. ⇒ JSR AT can improve the processability. 8 JSR Confidential Physical properties of vulcanized rubber i. Hardness & Elastic modulus ii. Vulcanized adhesion to steel cord iii. Vulcanized adhesion to Tread and Carcass iv. Durability(Heat resistance) 9 i. Hardness & Elastic modulus Hardness [Duro-A] Excellent Elastic modulus at 3% G’ Excellent JSR Confidential *Test mode ; Strain Dependence Temp=50℃ Frequency=100rad/sec Addition of AT provides high Hardness and high Elastic modulus. 10 JSR Confidential ii. Vulcanized adhesion to steel cord 【Test Method】 ・Steel cord : Brass plated cord Size : φ0.25mm×4 ・Cure Condition : 160℃×10min Steel cord ・Test speed : 50mm/min ← 650mm → ↑ Tension Compound Φ4mm ↓ Strength to pull out [Unit : N] Ref-1 NR only 1 AT300 2 AT400 Original 140 180 180 Heat cycle test 50times 160 170 190 Heat cycle test 100times 130 160 160 Run No. Ref-1 NR only 1 AT300 2 AT400 Original 100 125 120 Heat cycle test 50times 105 115 120 80 105 120 Run No. Amount of remaining rubber [INDEX] Heat cycle test 100times 【Heat cycle test】 1cycle : 0℃→Temperature rise at 5℃/min→30min Hold at 100℃→ Temperature drop at 5℃/min→30min Hold at 0℃ Addition of AT can improve the vulcanized adhesion to steel cord. 11 JSR Confidential iii. Vulcanized adhesion to Tread and Carcass Tension 15mm 4mm Tension 【Test Method】 ・Cure Condition : 160℃×10min ・Test speed : 50mm/min Peel Strength [Unit : N/15mm] Ref-1 NR only 1 AT300 2 AT400 Tread 120 140 130 Carcass 240 230 270 Run No. Tread;HP355R/BR01/1165MP/Si75/N339/OIL/Stearic acid/ZnO/6C/DPG/CZ/S=80/20/65/5.2/5/10/2/3/1/1.5/1.8/1.5 Carcass ; NR(RSS#3)/N330/OIL/Stearic acid/ZnO/6C/CZ/S=100/50/10/1/5/1/1/4 Vulcanized adhesion of compound with AT is as same as NR compound. 12 JSR Confidential iv. Durability(Heat resistance) *Test condition ; Temp=100℃ aging Tensile strength Excellent Hardness[Duro-A] Excellent Addition of AT provides good durability. ⇒ JSR AT can improve the physical properties of NR compound.13 JSR Confidential Summary ★Adding AT to NR compound can improve following properties. Decreases compound viscosity and increases flow rate. Excellent extrudability. Increases green strength and decreases mill shrinkage. High hardness and High Elastic modulus. High vulcanized adhesion to steel cord. Good durability. ☆NR compound with AT can improve following Tire properties. Processability(low compound viscosity) Driving stability(High hardness and modulus) High adhesive property of steel cord 14 Durability(Good Heat resistance)